Moisture content at packing is the only number that matters
Not the species, not the finish, not the kiln. The reading on the day the carton closes decides whether the chair is tight in year two.
Why packing and not drying
The kiln can bring timber to 8–10% at packing and a factory can still ship a frame at 13% if the parts sat in a humid machining hall for a week before assembly. Machined timber takes on moisture from the air in hours, and a workshop in Shunde in June is not a dry place.
So the number that matters is taken at packing, on the finished frame, not on the board that went into the kiln a month earlier. a container through the tropics can take 8% to 13% and back.
How it is measured
The pin meter on 20% of the batch, one cut test per kiln charge. The pin meter reads the top 2 mm, which on a lacquered frame is the finish rather than the timber, so it is taken on an unfinished part — a rail underside, a leg tenon, the inside of a back post.
The cut test is the honest one. Cut a 20 mm section, measure immediately, and compare it to the pin reading. The 2% gap between the two means the meter is reading the surface only, which is exactly how a wet core passes a pin test. Frames checked this way are on hotel dining chairs.
Writing it into the order
One line: moisture content at packing, 8–10%, measured by cut test, one piece per carton. That is checkable at the factory and at the hotel, and it costs nothing to add.
Where the number comes from and how it behaves in transit is the first section of the timber guide. Two notes that follow: kiln schedule and stress and end grain and water.
The packing side of the same problem is described under hotel furniture factory.