The timber guide: which species belongs on which part of a chair
Eight species by density, Janka and movement, and the part of the frame each one should be on. Start from the load, not from the look.
Start with the part, not the species
The chair is four jobs wearing one shape. The legs take compression and a bending moment at the floor. The back posts take the whole backward lean of a person. The seat rails take shear at the joints. The top, if there is one, takes abrasion and heat. Asking "which timber is best" without saying which of those four jobs you mean is why two buyers end up with different answers from the same factory.
So the question to put to a supplier is narrower: what species is on the back post, what is on the leg, what is under the seat, and what is the moisture content at packing. Those four answers tell you whether the price is honest. The range that comes out of this reasoning is on the hotel dining chairs page, and the tables that carry the widest solid stock are under hotel dining tables.
The eight species, by the numbers
| Species | Density | Janka | Belongs on |
|---|---|---|---|
| European beech | 700–750 kg/m³ | 1,300 | frame, legs, back posts, bent backs |
| Rubberwood | 600–650 kg/m³ | 1,000 | budget frames, rails, painted bodies |
| White oak | 750–770 kg/m³ | 1,360 | legs, aprons, tops, exposed frames |
| Ash | 650–700 kg/m³ | 1,320 | bent backs, arm bows, spindle backs |
| Black walnut | 640–660 kg/m³ | 1,010 | visible aprons, feature backs |
| Acacia | 700–750 kg/m³ | 1,700 | tops, seat slabs, covered terraces |
| Teak | 620–660 kg/m³ | 1,050 | terrace and poolside seating |
| Poplar | 400–450 kg/m³ | 540 | painted internal frames only |
Two numbers matter more than the rest. Density predicts how a leg wears at the floor contact. Janka predicts how the top survives a dropped plate. Neither predicts movement — that is the moisture section below, and it is the one that ruins more orders than hardness ever does.
Movement is the real specification
Timber moves across the grain as the room dries and swells with the season. Beech moves about about 0.4% per 1% moisture change across the grain. The dining room in a heated building in February sits near 25% relative humidity; the same room in July sits near 60%. That swing is wider than the kiln the timber came out of, which is why packing moisture — 8–10% at packing — is the number to write into the purchase order.
Two things follow. Anything wider than 120 mm should be a panel, not solid stock, or it will cup. And a joint that is glued tight at 13% moisture will open at 8%: not because the glue failed, but because the parts shrank away from each other. The joinery side of this is in the joinery guide, and the tables that carry the widest solid tops are on hotel dining tables.
What buyers get wrong
Three habits cost money. Asking for oak because a reference photo was oak: at 1,360 lbf it is hard, but the price moves with fashion and the grain is unforgiving on a turned leg. Asking for teak indoors because it sounds premium: right for rain, wrong for an indoor dining room at the price, and an indoor dining room never tests it. Putting poplar in a frame because the sample was painted: at 540 lbf it is furniture-board, not furniture.
The fourth habit is quieter. The buyer specifies beech, receives beech, and then finds the backs have been steam bent from a different species because the radius was too tight for the beech on hand. Tight radii belong to ash. If the drawing has a curve under 300 mm, say so in the specification and let the factory answer for the species it uses there.