The metal guide: wall thickness, welds and the salt spray number
Why 1.2 mm and 1.5 mm are different chairs, where rust starts on a welded frame, and what a 500 hour salt spray result actually proves.
Wall thickness is the whole argument
Two frames can look identical in a photograph and differ by 30% in steel. 1.2–1.5 mm is the range that holds a dining chair at EN 16139 level 2; below 1.2 mm the tube dents at the footrest before the weld ever complains. Buyers rarely see the difference until a chair comes back with a crease above the glide.
16–25 mm round, or 25 × 25 mm square Tube size follows the design, not the strength: a 16 mm round reads lighter than a 25 × 25 mm square, and a square section is easier to weld squarely. What matters is that the drawing states both, because "steel frame" on a quotation tells you nothing.
Where rust actually starts
Not on the flat faces. Rust starts at the weld seam, in the mill scale that was not removed before powder, and at the drilled hole where the seat pan bolts on. degrease, rinse, conversion coat, dry — four stages. Skip a stage and the powder goes on over a surface that was never converted, and it lifts in sheets eighteen months later.
The 1.2 mm wall takes 60–70 A on the MIG set. Push the current up to weld faster and the tube blows through; the welder patches it, the patch holds a stress riser, and the frame cracks next to the weld rather than at it. That is the failure you see as a hairline crack above the front leg.
What the salt spray number means
500 hours neutral salt spray on a coupon per batch. It is a coupon test, not a chair test: a flat plate of the same pre-treatment and the same powder, scribed and put in a fog chamber. It proves the process is under control. It does not prove the chair survives a seaside terrace, because the chair has edges, holes and crevices the coupon does not.
60–80 micron, cured at 180–200 °C. Thinner powder leaves the edges — where corrosion starts — with less cover than the face the gauge was pointed at. If a supplier quotes a salt spray figure without saying the film thickness, the figure is a brochure line.
Frames that pass all of this end up on hotel dining chairs and on counter stools, where the footrest takes the abuse.